Skin Depth Is Set by Resistivity, Not by Grade
A magnet answers one narrow question
Sorting scrap with a magnet is a blunt business, and the grades make it blunter. 201 is essentially nonmagnetic as annealed and becomes magnetic when cold worked, so a bent offcut sticks and a flat one does not. 302 is non-magnetic and cannot be hardened by heat treating, yet cold working makes it slightly magnetic. Alloy 625 is described as nonmagnetic while 17-7PH starts austenitic in the annealed state and picks up magnetic properties after ageing turns it to martensite. None of that tells a fabricator where an induction coil puts its heat, how deep a probe sees, or why a core is laminated. Those are questions about resistivity and permeability under an alternating field, and a pocket magnet answers neither.
The depth is a square root
Field penetrates a conductor by exponential decay, with a characteristic depth equal to the square root of resistivity over pi, frequency, free-space permeability and relative permeability. At 50 hertz the 825 data sheet gives a magnetic permeability of 1.005 at 200 oersteds and an electrical resistivity of 678 ohm circular mil per foot, which converts to about 1.13 microohm metres. Put those two numbers into the expression and the skin depth comes out at 75.5 millimetres. A coil at mains frequency barely notices a 6 mm wall of this alloy. The same sheet lists a thermal conductivity of 11.3 watts per metre kelvin at 26 degrees, and 904L quotes 12 W per metre kelvin at 20 degrees with a resistivity of 1.0 ohm square millimetre per metre. Low conductivity and high resistance travel together in these nickel-rich austenitics.
Magnetism divides that by thirty
The 430 page calls the grade a non-hardenable straight chromium steel in the ferritic group and tabulates 600 nanoohm metres of resistivity, with 409, also ferritic, at the same 600 and 25.8 W per metre kelvin. The page gives no permeability figure, so take 500 for a ferritic structure as a working assumption, not a certificate value. At 50 hertz that gives a skin depth of 2.47 mm against 75.5 mm for the austenitic alloy, a factor of thirty. The resistivity changed by less than two; the permeability did the rest. 420 is a hardenable martensitic modification of 410, and 416HT is martensitic, hardened by heat treatment and machined at about 85 per cent of free-cutting carbon steel. Both sit on the magnetic side of that divide.
Frequency is the dial the operator turns
Depth falls with the square root of frequency, so the coil, not the grade, sets the case depth. At 10 kilohertz the austenitic figure drops from 75.5 mm to 5.3 mm and the ferritic one from 2.47 mm to 0.17 mm. At 200 kilohertz they are 1.2 mm and 0.039 mm. A shop wanting a shallow hardened layer picks a high frequency and short dwell; it does not shop for a different alloy. 17-4PH lists electrical resistance of 0.71 ohm square millimetre per metre and states that magnetisability is available, while the annealed condition reaches very high yield strength after a low temperature treatment. The condition changes the permeability, and the condition belongs on the order.
The ladder printed on the data sheets
Reading the resistivity column across the range gives a twofold span rather than a single number: 550 nanoohm metres for 420, 600 for 430 and 409, 710 for 17-4PH, 800 for semi-austenitic 17-7PH, 940 for 310S, which reports 94 microhm centimetres at 20 degrees, 1000 for 904L, 1017 for fully austenitic 330, a grade not hardenable by heat treatment, and 1130 for 825. Thermal conductivity runs the other way: 304 is tabulated at 16.2 W per metre kelvin, 317LMN at 16.2, while 430 strip is credited with conductivity better than austenite and lower expansion. Multiplying the two gives roughly the same order in both families: alloying moves both at once.
Eddy loss is a thickness problem
For a sheet thinner than the skin depth, the eddy loss per unit volume goes as the square of flux density, frequency and thickness, divided by six times resistivity. At one tesla, 50 hertz and a 1 mm sheet, the arithmetic gives about 3.6 kilowatts per cubic metre for 825, 6.9 for 430 and 27 for a low carbon steel with a resistivity near 150 nanoohm metres. That is why a core is stacked from laminations below a millimetre rather than cut from solid: halving the thickness quarters the loss. The DC01 cold rolled sheet is offered specifically for electromagnetic properties as well as deep drawing, and 2205 duplex is noted for lower expansion and higher conductivity than austenitic grades. LDX 2101 balances ferrite and austenite in roughly equal amounts, and 2507 leans on its ferritic fraction; a mixed structure is a mixed electromagnetic answer too.
Why a thin tube is easy to inspect
Eddy-current testing works because a defect interrupts a current that is already flowing near the surface. On a thin wall the whole thickness sits inside the skin depth. On a heavy wall the centre is invisible and the frequency has to drop, which costs resolution. The A53 structural pipe allows a full body nondestructive electric test in place of the hydrostatic test on every length, and the stainless pipe programme lists squash, extended and water pressure checks alongside it. Square and rectangular hollow sections bring corner geometry into the same calculation, and 321 is non-magnetic in the annealed condition, so its permeability is close to unity and the probe reaches deeper than it would in a ferritic tube of the same wall.
Delivery condition moves the answer
Two pieces with the same grade name can sit on opposite sides of the divide. The 201 and 302 pages both say cold work brings on a magnetic response; 17-7PH is austenitic as annealed and martensitic in the hardened condition; the 17-4PH sheet says plainly that magnetisability is available; and stabilised 321 plate is supplied for high temperature service where the structure stays austenitic. 316 and 316L are austenitic and supplied passivated, and 317 takes a matching or higher molybdenum filler, which changes the seam's local structure. A permeability figure measured on annealed stock is not the figure on a formed, welded or aged component.
What the order has to say
If induction heating, eddy-current inspection, magnetic separation or shielding is in the job, write the frequency, the wall or sheet thickness, and the resistivity or the permeability you designed to. State the delivery condition and say whether cold work is permitted, because that alone can move a grade from one side of the divide to the other. Ask for the physical property table, not the grade name: the 825 sheet is useful because it prints permeability and resistivity together, and 904L gives both electrical and thermal figures. 254 SMO, 317 and 316L will all be quoted for corrosion first, but the coil on the bench reads none of that. It reads resistivity, permeability and frequency.
Next:No More!