A Hardness Number Is Not a Wear Rate
Three numbers on one certificate
A buyer comparing wearing parts usually gets a hardness figure and stops there. The catalogue makes that easy: 430 lists 183 Brinell maximum and 430F 262, 409 sits at 131 Brinell with a 75 Rockwell B ceiling, 302 plate carries a 201 Brinell ceiling with a 92 Rockwell B reading, and 422 is held to 290 Brinell maximum and 95 Rockwell B. Those are ceilings on a test, not rates of material loss. Put a part under a 500 newton normal load sliding 10 kilometres a year across a 1,000 square millimetre patch, with a dimensionless wear coefficient of one in ten thousand. That case shows how little the hardness column decides.
Archard is a division, not a specification
Wear volume is the coefficient times load times sliding distance, divided by hardness. Hardness in pascals is roughly 9.81 times the Brinell figure in megapascals, so 183 Brinell is about 1.80 gigapascals and 262 Brinell about 2.57. For the case above the arithmetic gives 0.5 divided by 1.80 billion, 278 cubic millimetres a year, against 195 for the harder grade. Spread over 1,000 square millimetres that is 0.279 mm against 0.195 mm of depth. A 43 per cent rise in hardness bought a 30 per cent cut in wear. Double the load and the volume doubles with no change in the metal. The surface treatment page says heat treatment improves hardness, wear resistance and strength, true and incomplete: it says nothing about load, distance or the coefficient.
The coefficient dwarfs the hardness
That coefficient is where the real spread lives. A well-lubricated steel pair can sit near one in a hundred thousand; a dry, grit-contaminated contact can reach one in a thousand, a hundredfold difference. Changing lubricant, counterface or sealing moves wear far more than moving up a grade. The wire rope page says it in trade language: grease is packed between rope and contact surface to reduce the wear rate and keep rust out, and the same rope range is sold for cranes and winches on that basis. 416HT is credited with low friction, which holds galling and seizing down, a wear statement built on friction rather than indentation. The 2205 sheet warns of rapid work hardening and higher forming forces, which describes the shop more than the service life.
Hertz pressure is set by geometry, not by grade
Put a 10 mm steel ball on a flat plate under the same 500 newtons. With a reduced modulus near 115 gigapascals the contact radius is 0.319 mm, a patch of 0.320 square millimetres. Average pressure is 1,563 MPa and the peak under the centre half as much again, near 2,344 MPa. Against the 310 MPa proof strength quoted for 430 that is more than seven times yield; the contact yields on the first pass whatever the certificate says. Hardness sets the load at which plastic flow starts, while geometry, load and modulus set the pressure that arrives. Even a part heat treated to Rockwell C45 in the H900 condition, against B85 in condition A, meets a pressure fixed elsewhere. 410 is a general purpose martensitic grade for highly stressed parts and 420 has carbon raised for hardness; both change the threshold, not the Hertz sum.
What a Brinell indentation actually samples
A Brinell reading comes from a 10 mm ball pressed under roughly 3,000 kilograms. The indentation is millimetres across and samples the bulk, while adhesive and abrasive wear happen in the first few micrometres. A coating can be harder or softer than the certificate number without appearing in it at all. The Z275 coil, rolled between 0.12 and 3 mm thick with Z60, Z80 and Z275 coating masses, carries roughly 19 micrometres of zinc on each face; a Brinell ball goes through that and reports the substrate. The light-gauge coil page splits tempers into three bands keyed to Rockwell B figures of 60, 60 through 85, and 85 through 95. Those bands describe how the sheet will form, not how long a sliding face will last.
Wear has more than one mechanism
Abrasive wear is hard particles ploughing a softer face, and there hardness helps in proportion. Adhesive wear is micro-welds tearing loose, where the pairing of two metals matters more than either number; the galling the 416HT sheet talks about. Repeated Hertz loading spalls a surface by fatigue, which needs toughness as much as hardness. Fretting works in tiny amplitudes at fitted joints, and erosion belongs to particles carried in a fluid. 430F carries a 0.15 per cent sulphur floor against a 0.030 ceiling on the plain 430, a screw-machine change that lowers corrosion resistance, not a wear upgrade. The 430 strip and the 422 grade with 897 MPa tensile and 207 MPa yield solve different problems, and one Brinell column cannot rank them across five mechanisms.
Cold work moves the number after you measured it
An annealed hardness is not the hardness of a worked surface. The 316L coil listing calls out excellent work hardening, and the 2205 sheet asks for a larger springback allowance because of high strength and rapid work hardening. A sliding or peened face hardens in service, so the value governing the second million cycles is not the value on the mill certificate. The 304L coil and the 316L grade sheet show the same austenitic behaviour from the chemistry side. Cold work also changes magnetism and corrosion response, so a treatment that buys wear life can quietly cost something else.
Roughness and the film between the surfaces
Whether a lubricant separates the two faces is a ratio of film thickness to combined roughness, not a hardness comparison. A ground face near 0.2 micrometres Ra and a rough machined face near 0.8 sit in different regimes under the same oil and load; below a ratio of one the asperities carry the load and the wear coefficient jumps by orders of magnitude. The 416HT sheet offers 2B, BA, No.4, HL, mirror and 8K finishes, which is a surface specification a buyer can order. The rope grease and the surface treatment routes act on the coefficient rather than on resistance to indentation.
What the order has to say instead
Name the mechanism first: abrasion, adhesion, contact fatigue, fretting or erosion. Give the counterface material and its condition, the normal load, the number of cycles and the sliding distance per cycle. Give the lubricant, the relubrication interval and the sealing that keeps grit out. State the surface roughness in Ra and the finish, the permitted wear depth before replacement, and the heat treatment condition behind any quoted hardness. Order Q235 or Q345 plate for the replaceable part with a cut blank leaving stock for finishing, and treat the 17-7PH data with its 330 MPa proof and 850 MPa tensile row as a starting point rather than a verdict. A hardness test is a cheap consistency check on delivered material. It is not a life prediction, and a drawing that specifies only 183 Brinell has specified almost nothing about how long the part will run.